Bearing failure analysis
More Grease Won’t Fix This Raceway
Evenly spaced lines across a dull grey raceway can mean electric current, not too little grease. Make four checks before a monthly regrease goes on the route.

In this article
The work order on the bench says “regrease monthly from now on”. Beside it lies the third bearing removed in a year from the non-drive end (NDE) of a fan motor. The motor in this worked example runs on a variable speed drive. The grease left in its cage pockets is dark and dry. Its outer raceway carries a dull grey band crossed by fine, evenly spaced lines.
The order assumes the grease failed first. If electric current cut those lines instead, a shorter interval adds labour and grease while the damage carries on, and SKF traces that damage through to spalling and even sudden seizure. Get it wrong the other way and the money goes on insulated bearings and filters while a lubrication fault stays in place.
So hold the order until four checks are in. Two of them can be made at the bench.
What drew the lines?
Play the odds and the regrease order looks right. SKF attributes about a third of bearing failures to lubrication problems and another third to contamination. ABB says bearing currents cause a very small number of motor bearing failures.
Evenly spaced lines are a different matter. SKF calls the pattern fluting and says it is most commonly attributed to damaging current passing through the bearing. On a motor run from a drive, the fast switching of the drive can raise a voltage on the shaft that breaks through the lubricant film. Repeated discharges pit the surface with tiny craters, and over time those craters can develop into flutes running parallel to the rolling axis.
Current can reach a bearing by more than one route, and the figure draws two. In larger motors, ABB explains, a voltage induced between the shaft ends can drive it round a loop through both bearings and the frame. In smaller motors shaft voltage can discharge across the grease film. The non-drive end, where this bearing came from, is where ABB puts an insulated bearing to break that loop.
The grease suffers too. Early in this failure it carbonises until it can no longer form a film, SKF notes, so the dark, dry grease fits the electrical picture without proving it. And there is a third candidate: vibration during operation can sometimes leave a similar washboard appearance.
Four checks, starting at the bench
The lines alone cannot settle it. Four checks narrow it down, nearest first.
| Check | Points towards current if you find | If you do not |
|---|---|---|
| The balls | Dull, light to dark grey over the whole surface | Bright balls weaken the electrical case |
| Bearing marking against the rating plate or maker’s data | An insulated bearing specified, a standard one fitted | Nothing either way |
| Cable, glands and bonding against the motor manual | Departures from the maker’s instructions | Nothing either way |
| The fluted band at 500× to 10,000× | Shallow, closely spaced craters | No craters: the electrical case weakens |
- Check
- The balls
- Points towards current if you find
- Dull, light to dark grey over the whole surface
- If you do not
- Bright balls weaken the electrical case
- Check
- Bearing marking against the rating plate or maker’s data
- Points towards current if you find
- An insulated bearing specified, a standard one fitted
- If you do not
- Nothing either way
- Check
- Cable, glands and bonding against the motor manual
- Points towards current if you find
- Departures from the maker’s instructions
- If you do not
- Nothing either way
- Check
- The fluted band at 500× to 10,000×
- Points towards current if you find
- Shallow, closely spaced craters
- If you do not
- No craters: the electrical case weakens
The first and last rows are evidence on the bearing. The middle two show only that current had a path.
Before anything is washed, bag a sample of the grease from the cage pockets. Then look at the balls. In this kind of damage, SKF says, they typically turn dull grey all over, light to dark.
Next, read the marking on the removed bearing against the motor’s rating plate, or against the maker’s data where a small motor’s plate does not list bearings. ABB, for example, shows the bearing insulation type on the plate, requires replacements of the same type and prohibits changing the insulation without its approval. A standard bearing fitted at this end at a repair can put the circulating loop back.
While the records are open, ask two questions. What did the drive-end bearing from the same motor look like? The same grey band at both ends would fit a current looping through both bearings and the frame. One end only does not rule it out. And when did the failures start? ABB’s drives guide describes bearing failures from electrical discharge machining (EDM) appearing within one to six months of start-up, so set the dates against the day the drive was fitted and any repair.
Then walk the installation with the motor manual in hand. For its motors on converter supply, ABB requires shielded symmetrical cable and 360° glands above 30 kW and highly recommends the same cable for smaller ones.
The slowest check is the ring itself, so start it today. SKF says the craters can hardly be seen without magnification and suggests 500× to 10,000× to confirm them. A hand magnifier shows the pattern, not the craters, so send the ring and the grease sample to the bearing supplier or a failure-analysis laboratory.
What to do with the regrease order this week
On a fan that runs around the clock, monthly means about 730 running hours between greasings (8,760 h ÷ 12). Compare that with the interval on the motor’s lubrication plate; ABB sets its plate values for the mounting, ambient temperature and speed. A drive can justify a shorter interval: ABB says higher speed operation, as in converter applications, or low speed with heavy load needs shorter intervals. That case rests on speed and load, not on the pattern in a failed raceway.
So keep the plate interval for the speed the drive actually runs, and hold the monthly order until the checks are in. While the ring is away, have the route check both motor bearings for noise, vibration and temperature at every visit: if current is the cause, the replacement is exposed to it now. On the order itself, write what is still open: “Monthly regrease on hold. NDE ring and grease sample at the laboratory. Bearing marking and cabling to check.”
If the laboratory finds no craters and the balls are bright, the electrical case weakens. Go back to the questions behind SKF’s lubrication and contamination figures (which grease, how much, how often, how clean) and look at the vibration history before anyone changes the route.
If craters are confirmed, the fix belongs in the bearing specification and the electrical installation, and the order matters. Start with the installation: SKF’s first action for fluting is to check the grounding, and ABB puts earthing and shielded symmetrical cabling (3 in the figure) ahead of a filter. Then restore what the rating plate specifies, an insulated bearing where one belongs (1). Only if both are already right is it time for a specialist measurement, which ABB says takes special equipment, experienced personnel and a motor running at no less than 10 per cent of nominal speed so that the balls ride on the film. What remains depends on the route the current takes: SKF lists an insulated or hybrid bearing or an insulating sleeve, ABB a shaft grounding brush (2) and, on large motors, a common-mode filter. Have the motor maker approve the choice.
No fix here is a shorter regreasing interval.
References
- SKF, Bearing damage and failure analysis (PUB BU/I3 14219/3 EN, June 2025), Table 2 solution code 41, page 28 (PDF). Magnifying 500× to 10,000× to confirm craters, fluting most commonly attributed to current, a washboard appearance that vibration can leave, and SKF’s corrective actions; page 6 gives the one-third shares for lubrication and contamination.
- SKF, Bearing damage and failure analysis, section 5.4.3 Current leakage erosion and Fig. 34, pages 54 to 55 (PDF). Shallow craters that develop into flutes parallel to the rolling axis, dull grey balls, and grease that carbonises and stops forming a film.
- ABB, Bearing currents and their mitigation, product note 9AKK107336 EN 06-2018 (PDF). Shaft voltage breaking through the lubricant film, the three types of bearing current, the mitigation options, specialist measurement, and the small share of failures caused by bearing currents.
- ABB, Low voltage motors manual 3GZF500730-85 Rev H (05-2022), sections 6.1, 6.4, 6.5, 7.1, 7.2, 7.2.2, 7.2.3 and 8.3, pages 15 to 23 (PDF). Bearing insulation and bearing types on the rating plate (except smaller frame sizes), same-type replacement bearings, shielded symmetrical cable with 360° glands for motors on converter supply, and lubrication intervals set by the plate and shortened for higher converter speeds or low speed with heavy load.
- ABB, Technical guide No. 5, Bearing currents in modern AC drive systems (3AFE64230247 Rev C), chapters 2 and 3, in Technical guide book 3AFE64514482 Rev H (PDF). How circulating and capacitive discharge currents arise, how cabling, insulation and filtering act on them, the failures reported within one to six months of start-up, and the running-speed condition for specialist measurement.